Indentation-Induced Failure of Hard Coatings

                                                            Adnan Abdul-Baqi & Erik van der Giessen
                                                                                           Koiter Institute Delft

                                                                                                                              F
Introduction




                                                                                                                                                                                                                )
                                                                                                                                                                                                                 max
                                                                                                                          O       R             r




                                                                                                                                                                                                                (τ
Indentation-induced failure of hard coatings is modelled by means of                                                 h        a                          Film (elastic)             t




                                                                                                                                                                                                                 max
                                                                                                                                                                                                                                    normal




                                                                                                                                                                                                            σ
cohesive surfaces. Interfacial delamination (normal & shear) and                                                                                                Interface
coating cracking are the failure events being under consideration.                                                    z                                                                                                         shear




                                                                                                     Symmetry axis
For the cohesive surface, the constitutive behaviour is given in terms                                                                 Substrate (elastic-plastic)                                                                            ∆ (∆ )
                                                                                                                                                                                                                                               n       t
of a traction versus separation law, where we have adopted the uni-
versal binding law used by Xu and Needleman [1]. It is characterized
mainly by the peak traction and the separation energy (Fig. 2).


Results                                                                                                                   Figure 1. Geometry.                                                    Figure 2. Cohesive zone tractions. The
                                                                                                                                                                                                 energy for normal or shear separation is
                                                                                                                                                                                                 the area under the corresponding curve.
  Interfacial delamination:

           0                                           σe/σy                  0                                                                                                             1
                                                                                                                                                     σzz/σmax
                                                                 1.40                                                                                           1.00
                                                                 1.20                                                                                                                              shear delamination
                                                                                                                                                                0.75                       0.8     normal delamination
                                                                 1.00                                                                                           0.50
    50                                                           0.80      20
                                                                                                                                                                0.25
                                                                 0.60                                                                                                                      0.6




                                                                                                                                                                                  F/Fmax
                                                                                                                                                                 0.00
                                                                         z (µm)
  z (µm)




                                                                 0.40                                                                                           -0.25
                                                                 0.20                                                                                           -0.50                      0.4
  100                                                                      40

                                                                                                                                                                                           0.2


                                                                                                                                                         (b)                                0
  150                                                      (a)             60                                                                                                                0            0.5              1            1.5                 2
               0           50             100        150                          0             20                                40            60                                                                        h/t
                                r (µm)                                                                               r (µm)
  Figure 3. (a) Shear delamination . t = 5 µm, τ max = 1.2 GPa . Arrows show the shear direction, line                                                                            Figure 4. Load versus displacement (F-h) curves for
  shows the location of the delaminated area. (b) Normal delamination. t = 2.5 µm, σ max = 1.5 GPa .                                                                              Fig. 3.




   Coating cracking:

               0                                                                   0
                                                          σrr/σmax                                                                                       σrr/σmax                    1
                                                                                                                                                                                                                                                   e
                                                                 2.00                                                                                            2.00
                                                                 1.56                                                                                            1.56                                                                   d
               5
                                                                                                                                                                                  0.8
                                                                 1.11              5                                                                             1.11
                                                                  0.67                                                                                           0.67
                                                                  0.22                                                                                           0.22             0.6
                                                                                                                                                                         F/Fmax
   z (µm)




                                                                         z (µm)




            10                                                   -0.22            10                                                                            -0.22                                                  b c
                                                                 -0.67                                                                                          -0.67             0.4
                                                                 -1.11                                                                                          -1.11
                                                                                                                                                                                                      a
            15                                                   -1.56            15                                                                            -1.56
                                                                 -2.00                                                                                          -2.00             0.2


            20                                             (a)                    20                                                                      (b)                        0
                   0   5           10           15   20                                0    5                              10          15           20                                0                    0.5                  1                          1.5
                                 r (µm)                                                                                  r (µm)                                                                                         h/t
  Figure 5. Coating cracking. t = 2 µm, σ max = 11 GPa . (a) First crack at r 1 = 7.0 µm . (b) Second                                                                    Figure 6. Load versus displacement curve for Fig. 5.
  crack at r 2 = 9.4 µm .                                                                                                                                                Labelled points correspond to specific failure types. a
                                                                                                                                                                         and b on the curve correspond to mode I cracks at loca-
                                                                                                                                                                         tions r 1 and r 2 , respectively. At c the first crack grows
Conclusions                                                                                                                                                              until the interface and at d it shears of f. Point e corre-
                                                                                                                                                                         sponds to some limited interfacial delamination in the
1. Shear delamination may occur in the loading stage. It is imprinted on the load vs displacement curve by a kink.                                                       vicinity of the coating cracks.

2. Normal delamination may occur during the unloading stage, where a circular part of the coating is lifted off
from the substrate. It is imprinted on the load vs displacement curve by a hump.

3. Coating cracking may occur during the loading stage. The first circumferential crack occurs outside the con-
tact area. The crack is imprinted on the F-h curve as a kink.

4. On further loading, subsequent cracking occurs with crack spacing of about 1.25 times the coating thickness.                                                         [1] X.-P. Xu, A. Needleman, Model. Simul. Mater. Sci. Eng. 1 (1993) 111.

Más contenido relacionado

La actualidad más candente

John Butler Poster 2011
John Butler Poster 2011John Butler Poster 2011
John Butler Poster 2011johnbutler1977
 
Shrikage behavior of UHPC
Shrikage behavior of UHPCShrikage behavior of UHPC
Shrikage behavior of UHPCsupercrete
 
Avoidance of Microstructural Heterogeneities by Hot Rolling Design in Thin Sl...
Avoidance of Microstructural Heterogeneities by Hot Rolling Design in Thin Sl...Avoidance of Microstructural Heterogeneities by Hot Rolling Design in Thin Sl...
Avoidance of Microstructural Heterogeneities by Hot Rolling Design in Thin Sl...Pello Uranga
 
Role of Microalloying Elements during Thin Slab Direct Rolling
Role of Microalloying Elements during Thin Slab Direct RollingRole of Microalloying Elements during Thin Slab Direct Rolling
Role of Microalloying Elements during Thin Slab Direct RollingPello Uranga
 
Optimization of Rolling Conditions in Nb Microalloyed Steels Processed by Thi...
Optimization of Rolling Conditions in Nb Microalloyed Steels Processed by Thi...Optimization of Rolling Conditions in Nb Microalloyed Steels Processed by Thi...
Optimization of Rolling Conditions in Nb Microalloyed Steels Processed by Thi...Pello Uranga
 
Modal and harmonic analysis of tapered composite i
Modal and harmonic analysis of tapered composite iModal and harmonic analysis of tapered composite i
Modal and harmonic analysis of tapered composite iSRINIVASULU N V
 
Study of Metadynamic Recrystallization Phenomena in Coarse Grained Nb Microal...
Study of Metadynamic Recrystallization Phenomena in Coarse Grained Nb Microal...Study of Metadynamic Recrystallization Phenomena in Coarse Grained Nb Microal...
Study of Metadynamic Recrystallization Phenomena in Coarse Grained Nb Microal...Pello Uranga
 

La actualidad más candente (12)

Session 29 ic2011 gereke
Session 29 ic2011 gerekeSession 29 ic2011 gereke
Session 29 ic2011 gereke
 
The speed paradigm
The speed paradigmThe speed paradigm
The speed paradigm
 
John Butler Poster 2011
John Butler Poster 2011John Butler Poster 2011
John Butler Poster 2011
 
TE-DM20B-8H3
TE-DM20B-8H3TE-DM20B-8H3
TE-DM20B-8H3
 
Shrikage behavior of UHPC
Shrikage behavior of UHPCShrikage behavior of UHPC
Shrikage behavior of UHPC
 
Avoidance of Microstructural Heterogeneities by Hot Rolling Design in Thin Sl...
Avoidance of Microstructural Heterogeneities by Hot Rolling Design in Thin Sl...Avoidance of Microstructural Heterogeneities by Hot Rolling Design in Thin Sl...
Avoidance of Microstructural Heterogeneities by Hot Rolling Design in Thin Sl...
 
Quenching, surface treatment and hardness tests
Quenching, surface treatment and hardness testsQuenching, surface treatment and hardness tests
Quenching, surface treatment and hardness tests
 
Role of Microalloying Elements during Thin Slab Direct Rolling
Role of Microalloying Elements during Thin Slab Direct RollingRole of Microalloying Elements during Thin Slab Direct Rolling
Role of Microalloying Elements during Thin Slab Direct Rolling
 
Optimization of Rolling Conditions in Nb Microalloyed Steels Processed by Thi...
Optimization of Rolling Conditions in Nb Microalloyed Steels Processed by Thi...Optimization of Rolling Conditions in Nb Microalloyed Steels Processed by Thi...
Optimization of Rolling Conditions in Nb Microalloyed Steels Processed by Thi...
 
Modal and harmonic analysis of tapered composite i
Modal and harmonic analysis of tapered composite iModal and harmonic analysis of tapered composite i
Modal and harmonic analysis of tapered composite i
 
TE-DL18A-4H7.8
TE-DL18A-4H7.8TE-DL18A-4H7.8
TE-DL18A-4H7.8
 
Study of Metadynamic Recrystallization Phenomena in Coarse Grained Nb Microal...
Study of Metadynamic Recrystallization Phenomena in Coarse Grained Nb Microal...Study of Metadynamic Recrystallization Phenomena in Coarse Grained Nb Microal...
Study of Metadynamic Recrystallization Phenomena in Coarse Grained Nb Microal...
 

Destacado

delamination of a strong film from a ductile substrate during indentation unl...
delamination of a strong film from a ductile substrate during indentation unl...delamination of a strong film from a ductile substrate during indentation unl...
delamination of a strong film from a ductile substrate during indentation unl...Dr. Adnan Judeh (Abdul-Baqi)
 
M.Sc. Thesis - Atomic Physics Aspects of Radiation Physics
M.Sc. Thesis - Atomic Physics Aspects of Radiation PhysicsM.Sc. Thesis - Atomic Physics Aspects of Radiation Physics
M.Sc. Thesis - Atomic Physics Aspects of Radiation PhysicsDr. Adnan Judeh (Abdul-Baqi)
 
Environment Quality Authority (EQA) standards and regulations for monitoring ...
Environment Quality Authority (EQA) standards and regulations for monitoring ...Environment Quality Authority (EQA) standards and regulations for monitoring ...
Environment Quality Authority (EQA) standards and regulations for monitoring ...Dr. Adnan Judeh (Abdul-Baqi)
 
Many electrons atoms_2012.12.04 (PDF with links
Many electrons atoms_2012.12.04 (PDF with linksMany electrons atoms_2012.12.04 (PDF with links
Many electrons atoms_2012.12.04 (PDF with linksLadislav Kocbach
 
Radiation emitted from Israeli mobile base-stations (in Arabic with English a...
Radiation emitted from Israeli mobile base-stations (in Arabic with English a...Radiation emitted from Israeli mobile base-stations (in Arabic with English a...
Radiation emitted from Israeli mobile base-stations (in Arabic with English a...Dr. Adnan Judeh (Abdul-Baqi)
 
Radiation emitted from Israeli mobile base-stations
Radiation emitted from Israeli mobile base-stationsRadiation emitted from Israeli mobile base-stations
Radiation emitted from Israeli mobile base-stationsDr. Adnan Judeh (Abdul-Baqi)
 
Ph.D. Thesis - Failure of Brittle Coatings on Ductile Metallic Substrates
Ph.D. Thesis - Failure of Brittle Coatings on Ductile Metallic SubstratesPh.D. Thesis - Failure of Brittle Coatings on Ductile Metallic Substrates
Ph.D. Thesis - Failure of Brittle Coatings on Ductile Metallic SubstratesDr. Adnan Judeh (Abdul-Baqi)
 

Destacado (10)

delamination of a strong film from a ductile substrate during indentation unl...
delamination of a strong film from a ductile substrate during indentation unl...delamination of a strong film from a ductile substrate during indentation unl...
delamination of a strong film from a ductile substrate during indentation unl...
 
M.Sc. Thesis - Atomic Physics Aspects of Radiation Physics
M.Sc. Thesis - Atomic Physics Aspects of Radiation PhysicsM.Sc. Thesis - Atomic Physics Aspects of Radiation Physics
M.Sc. Thesis - Atomic Physics Aspects of Radiation Physics
 
Environment Quality Authority (EQA) standards and regulations for monitoring ...
Environment Quality Authority (EQA) standards and regulations for monitoring ...Environment Quality Authority (EQA) standards and regulations for monitoring ...
Environment Quality Authority (EQA) standards and regulations for monitoring ...
 
Fatigue damage - poster
Fatigue damage - posterFatigue damage - poster
Fatigue damage - poster
 
Delamination of thin strong film - poster
Delamination of thin strong film  - posterDelamination of thin strong film  - poster
Delamination of thin strong film - poster
 
Many electrons atoms_2012.12.04 (PDF with links
Many electrons atoms_2012.12.04 (PDF with linksMany electrons atoms_2012.12.04 (PDF with links
Many electrons atoms_2012.12.04 (PDF with links
 
Guidlines of the ICNIRP on radiowaves
Guidlines of the ICNIRP on radiowavesGuidlines of the ICNIRP on radiowaves
Guidlines of the ICNIRP on radiowaves
 
Radiation emitted from Israeli mobile base-stations (in Arabic with English a...
Radiation emitted from Israeli mobile base-stations (in Arabic with English a...Radiation emitted from Israeli mobile base-stations (in Arabic with English a...
Radiation emitted from Israeli mobile base-stations (in Arabic with English a...
 
Radiation emitted from Israeli mobile base-stations
Radiation emitted from Israeli mobile base-stationsRadiation emitted from Israeli mobile base-stations
Radiation emitted from Israeli mobile base-stations
 
Ph.D. Thesis - Failure of Brittle Coatings on Ductile Metallic Substrates
Ph.D. Thesis - Failure of Brittle Coatings on Ductile Metallic SubstratesPh.D. Thesis - Failure of Brittle Coatings on Ductile Metallic Substrates
Ph.D. Thesis - Failure of Brittle Coatings on Ductile Metallic Substrates
 

Más de Dr. Adnan Judeh (Abdul-Baqi)

Lecture on radiation emitted from mobile base-stations at Tulkarim 19-2-2014
Lecture on radiation emitted from mobile base-stations at Tulkarim 19-2-2014Lecture on radiation emitted from mobile base-stations at Tulkarim 19-2-2014
Lecture on radiation emitted from mobile base-stations at Tulkarim 19-2-2014Dr. Adnan Judeh (Abdul-Baqi)
 
Radiation emitted from mobile base-stations (presentation in Arabic)
Radiation emitted from mobile base-stations (presentation in Arabic)Radiation emitted from mobile base-stations (presentation in Arabic)
Radiation emitted from mobile base-stations (presentation in Arabic)Dr. Adnan Judeh (Abdul-Baqi)
 
Fatigue damage in solder joint interconnects - presentation
Fatigue damage in solder joint interconnects - presentationFatigue damage in solder joint interconnects - presentation
Fatigue damage in solder joint interconnects - presentationDr. Adnan Judeh (Abdul-Baqi)
 
radiation emitted from mobile base-stations (article in Arabic)
radiation emitted from mobile base-stations (article in Arabic)radiation emitted from mobile base-stations (article in Arabic)
radiation emitted from mobile base-stations (article in Arabic)Dr. Adnan Judeh (Abdul-Baqi)
 
simulation of fatigue damage in solder joints using cohesive zones
simulation of fatigue damage in solder joints using cohesive zonessimulation of fatigue damage in solder joints using cohesive zones
simulation of fatigue damage in solder joints using cohesive zonesDr. Adnan Judeh (Abdul-Baqi)
 
study of environmental radioactivity in Palestine by in situ gamma-ray spectr...
study of environmental radioactivity in Palestine by in situ gamma-ray spectr...study of environmental radioactivity in Palestine by in situ gamma-ray spectr...
study of environmental radioactivity in Palestine by in situ gamma-ray spectr...Dr. Adnan Judeh (Abdul-Baqi)
 
fatigue damage modeling in solder interconnects using a cohesive zone approach
fatigue damage modeling in solder interconnects using a cohesive zone approachfatigue damage modeling in solder interconnects using a cohesive zone approach
fatigue damage modeling in solder interconnects using a cohesive zone approachDr. Adnan Judeh (Abdul-Baqi)
 
numerical analysis of indentation-induced cracking of brittle coatings on duc...
numerical analysis of indentation-induced cracking of brittle coatings on duc...numerical analysis of indentation-induced cracking of brittle coatings on duc...
numerical analysis of indentation-induced cracking of brittle coatings on duc...Dr. Adnan Judeh (Abdul-Baqi)
 
Indentation-induced interface delamination of a strong film on a ductile subs...
Indentation-induced interface delamination of a strong film on a ductile subs...Indentation-induced interface delamination of a strong film on a ductile subs...
Indentation-induced interface delamination of a strong film on a ductile subs...Dr. Adnan Judeh (Abdul-Baqi)
 

Más de Dr. Adnan Judeh (Abdul-Baqi) (10)

Lecture on radiation emitted from mobile base-stations at Tulkarim 19-2-2014
Lecture on radiation emitted from mobile base-stations at Tulkarim 19-2-2014Lecture on radiation emitted from mobile base-stations at Tulkarim 19-2-2014
Lecture on radiation emitted from mobile base-stations at Tulkarim 19-2-2014
 
Radiation emitted from mobile base-stations (presentation in Arabic)
Radiation emitted from mobile base-stations (presentation in Arabic)Radiation emitted from mobile base-stations (presentation in Arabic)
Radiation emitted from mobile base-stations (presentation in Arabic)
 
Fatigue damage in solder joint interconnects - presentation
Fatigue damage in solder joint interconnects - presentationFatigue damage in solder joint interconnects - presentation
Fatigue damage in solder joint interconnects - presentation
 
CV - Adnan
CV - AdnanCV - Adnan
CV - Adnan
 
radiation emitted from mobile base-stations (article in Arabic)
radiation emitted from mobile base-stations (article in Arabic)radiation emitted from mobile base-stations (article in Arabic)
radiation emitted from mobile base-stations (article in Arabic)
 
simulation of fatigue damage in solder joints using cohesive zones
simulation of fatigue damage in solder joints using cohesive zonessimulation of fatigue damage in solder joints using cohesive zones
simulation of fatigue damage in solder joints using cohesive zones
 
study of environmental radioactivity in Palestine by in situ gamma-ray spectr...
study of environmental radioactivity in Palestine by in situ gamma-ray spectr...study of environmental radioactivity in Palestine by in situ gamma-ray spectr...
study of environmental radioactivity in Palestine by in situ gamma-ray spectr...
 
fatigue damage modeling in solder interconnects using a cohesive zone approach
fatigue damage modeling in solder interconnects using a cohesive zone approachfatigue damage modeling in solder interconnects using a cohesive zone approach
fatigue damage modeling in solder interconnects using a cohesive zone approach
 
numerical analysis of indentation-induced cracking of brittle coatings on duc...
numerical analysis of indentation-induced cracking of brittle coatings on duc...numerical analysis of indentation-induced cracking of brittle coatings on duc...
numerical analysis of indentation-induced cracking of brittle coatings on duc...
 
Indentation-induced interface delamination of a strong film on a ductile subs...
Indentation-induced interface delamination of a strong film on a ductile subs...Indentation-induced interface delamination of a strong film on a ductile subs...
Indentation-induced interface delamination of a strong film on a ductile subs...
 

Último

Apidays New York 2024 - The value of a flexible API Management solution for O...
Apidays New York 2024 - The value of a flexible API Management solution for O...Apidays New York 2024 - The value of a flexible API Management solution for O...
Apidays New York 2024 - The value of a flexible API Management solution for O...apidays
 
A Year of the Servo Reboot: Where Are We Now?
A Year of the Servo Reboot: Where Are We Now?A Year of the Servo Reboot: Where Are We Now?
A Year of the Servo Reboot: Where Are We Now?Igalia
 
Understanding Discord NSFW Servers A Guide for Responsible Users.pdf
Understanding Discord NSFW Servers A Guide for Responsible Users.pdfUnderstanding Discord NSFW Servers A Guide for Responsible Users.pdf
Understanding Discord NSFW Servers A Guide for Responsible Users.pdfUK Journal
 
[2024]Digital Global Overview Report 2024 Meltwater.pdf
[2024]Digital Global Overview Report 2024 Meltwater.pdf[2024]Digital Global Overview Report 2024 Meltwater.pdf
[2024]Digital Global Overview Report 2024 Meltwater.pdfhans926745
 
Driving Behavioral Change for Information Management through Data-Driven Gree...
Driving Behavioral Change for Information Management through Data-Driven Gree...Driving Behavioral Change for Information Management through Data-Driven Gree...
Driving Behavioral Change for Information Management through Data-Driven Gree...Enterprise Knowledge
 
Automating Google Workspace (GWS) & more with Apps Script
Automating Google Workspace (GWS) & more with Apps ScriptAutomating Google Workspace (GWS) & more with Apps Script
Automating Google Workspace (GWS) & more with Apps Scriptwesley chun
 
Handwritten Text Recognition for manuscripts and early printed texts
Handwritten Text Recognition for manuscripts and early printed textsHandwritten Text Recognition for manuscripts and early printed texts
Handwritten Text Recognition for manuscripts and early printed textsMaria Levchenko
 
AWS Community Day CPH - Three problems of Terraform
AWS Community Day CPH - Three problems of TerraformAWS Community Day CPH - Three problems of Terraform
AWS Community Day CPH - Three problems of TerraformAndrey Devyatkin
 
Scaling API-first – The story of a global engineering organization
Scaling API-first – The story of a global engineering organizationScaling API-first – The story of a global engineering organization
Scaling API-first – The story of a global engineering organizationRadu Cotescu
 
Strategies for Unlocking Knowledge Management in Microsoft 365 in the Copilot...
Strategies for Unlocking Knowledge Management in Microsoft 365 in the Copilot...Strategies for Unlocking Knowledge Management in Microsoft 365 in the Copilot...
Strategies for Unlocking Knowledge Management in Microsoft 365 in the Copilot...Drew Madelung
 
Real Time Object Detection Using Open CV
Real Time Object Detection Using Open CVReal Time Object Detection Using Open CV
Real Time Object Detection Using Open CVKhem
 
A Domino Admins Adventures (Engage 2024)
A Domino Admins Adventures (Engage 2024)A Domino Admins Adventures (Engage 2024)
A Domino Admins Adventures (Engage 2024)Gabriella Davis
 
Boost Fertility New Invention Ups Success Rates.pdf
Boost Fertility New Invention Ups Success Rates.pdfBoost Fertility New Invention Ups Success Rates.pdf
Boost Fertility New Invention Ups Success Rates.pdfsudhanshuwaghmare1
 
Artificial Intelligence: Facts and Myths
Artificial Intelligence: Facts and MythsArtificial Intelligence: Facts and Myths
Artificial Intelligence: Facts and MythsJoaquim Jorge
 
The 7 Things I Know About Cyber Security After 25 Years | April 2024
The 7 Things I Know About Cyber Security After 25 Years | April 2024The 7 Things I Know About Cyber Security After 25 Years | April 2024
The 7 Things I Know About Cyber Security After 25 Years | April 2024Rafal Los
 
How to Troubleshoot Apps for the Modern Connected Worker
How to Troubleshoot Apps for the Modern Connected WorkerHow to Troubleshoot Apps for the Modern Connected Worker
How to Troubleshoot Apps for the Modern Connected WorkerThousandEyes
 
Histor y of HAM Radio presentation slide
Histor y of HAM Radio presentation slideHistor y of HAM Radio presentation slide
Histor y of HAM Radio presentation slidevu2urc
 
Bajaj Allianz Life Insurance Company - Insurer Innovation Award 2024
Bajaj Allianz Life Insurance Company - Insurer Innovation Award 2024Bajaj Allianz Life Insurance Company - Insurer Innovation Award 2024
Bajaj Allianz Life Insurance Company - Insurer Innovation Award 2024The Digital Insurer
 
Axa Assurance Maroc - Insurer Innovation Award 2024
Axa Assurance Maroc - Insurer Innovation Award 2024Axa Assurance Maroc - Insurer Innovation Award 2024
Axa Assurance Maroc - Insurer Innovation Award 2024The Digital Insurer
 
🐬 The future of MySQL is Postgres 🐘
🐬  The future of MySQL is Postgres   🐘🐬  The future of MySQL is Postgres   🐘
🐬 The future of MySQL is Postgres 🐘RTylerCroy
 

Último (20)

Apidays New York 2024 - The value of a flexible API Management solution for O...
Apidays New York 2024 - The value of a flexible API Management solution for O...Apidays New York 2024 - The value of a flexible API Management solution for O...
Apidays New York 2024 - The value of a flexible API Management solution for O...
 
A Year of the Servo Reboot: Where Are We Now?
A Year of the Servo Reboot: Where Are We Now?A Year of the Servo Reboot: Where Are We Now?
A Year of the Servo Reboot: Where Are We Now?
 
Understanding Discord NSFW Servers A Guide for Responsible Users.pdf
Understanding Discord NSFW Servers A Guide for Responsible Users.pdfUnderstanding Discord NSFW Servers A Guide for Responsible Users.pdf
Understanding Discord NSFW Servers A Guide for Responsible Users.pdf
 
[2024]Digital Global Overview Report 2024 Meltwater.pdf
[2024]Digital Global Overview Report 2024 Meltwater.pdf[2024]Digital Global Overview Report 2024 Meltwater.pdf
[2024]Digital Global Overview Report 2024 Meltwater.pdf
 
Driving Behavioral Change for Information Management through Data-Driven Gree...
Driving Behavioral Change for Information Management through Data-Driven Gree...Driving Behavioral Change for Information Management through Data-Driven Gree...
Driving Behavioral Change for Information Management through Data-Driven Gree...
 
Automating Google Workspace (GWS) & more with Apps Script
Automating Google Workspace (GWS) & more with Apps ScriptAutomating Google Workspace (GWS) & more with Apps Script
Automating Google Workspace (GWS) & more with Apps Script
 
Handwritten Text Recognition for manuscripts and early printed texts
Handwritten Text Recognition for manuscripts and early printed textsHandwritten Text Recognition for manuscripts and early printed texts
Handwritten Text Recognition for manuscripts and early printed texts
 
AWS Community Day CPH - Three problems of Terraform
AWS Community Day CPH - Three problems of TerraformAWS Community Day CPH - Three problems of Terraform
AWS Community Day CPH - Three problems of Terraform
 
Scaling API-first – The story of a global engineering organization
Scaling API-first – The story of a global engineering organizationScaling API-first – The story of a global engineering organization
Scaling API-first – The story of a global engineering organization
 
Strategies for Unlocking Knowledge Management in Microsoft 365 in the Copilot...
Strategies for Unlocking Knowledge Management in Microsoft 365 in the Copilot...Strategies for Unlocking Knowledge Management in Microsoft 365 in the Copilot...
Strategies for Unlocking Knowledge Management in Microsoft 365 in the Copilot...
 
Real Time Object Detection Using Open CV
Real Time Object Detection Using Open CVReal Time Object Detection Using Open CV
Real Time Object Detection Using Open CV
 
A Domino Admins Adventures (Engage 2024)
A Domino Admins Adventures (Engage 2024)A Domino Admins Adventures (Engage 2024)
A Domino Admins Adventures (Engage 2024)
 
Boost Fertility New Invention Ups Success Rates.pdf
Boost Fertility New Invention Ups Success Rates.pdfBoost Fertility New Invention Ups Success Rates.pdf
Boost Fertility New Invention Ups Success Rates.pdf
 
Artificial Intelligence: Facts and Myths
Artificial Intelligence: Facts and MythsArtificial Intelligence: Facts and Myths
Artificial Intelligence: Facts and Myths
 
The 7 Things I Know About Cyber Security After 25 Years | April 2024
The 7 Things I Know About Cyber Security After 25 Years | April 2024The 7 Things I Know About Cyber Security After 25 Years | April 2024
The 7 Things I Know About Cyber Security After 25 Years | April 2024
 
How to Troubleshoot Apps for the Modern Connected Worker
How to Troubleshoot Apps for the Modern Connected WorkerHow to Troubleshoot Apps for the Modern Connected Worker
How to Troubleshoot Apps for the Modern Connected Worker
 
Histor y of HAM Radio presentation slide
Histor y of HAM Radio presentation slideHistor y of HAM Radio presentation slide
Histor y of HAM Radio presentation slide
 
Bajaj Allianz Life Insurance Company - Insurer Innovation Award 2024
Bajaj Allianz Life Insurance Company - Insurer Innovation Award 2024Bajaj Allianz Life Insurance Company - Insurer Innovation Award 2024
Bajaj Allianz Life Insurance Company - Insurer Innovation Award 2024
 
Axa Assurance Maroc - Insurer Innovation Award 2024
Axa Assurance Maroc - Insurer Innovation Award 2024Axa Assurance Maroc - Insurer Innovation Award 2024
Axa Assurance Maroc - Insurer Innovation Award 2024
 
🐬 The future of MySQL is Postgres 🐘
🐬  The future of MySQL is Postgres   🐘🐬  The future of MySQL is Postgres   🐘
🐬 The future of MySQL is Postgres 🐘
 

Indentation induced failure - poster

  • 1. Indentation-Induced Failure of Hard Coatings Adnan Abdul-Baqi & Erik van der Giessen Koiter Institute Delft F Introduction ) max O R r (τ Indentation-induced failure of hard coatings is modelled by means of h a Film (elastic) t max normal σ cohesive surfaces. Interfacial delamination (normal & shear) and Interface coating cracking are the failure events being under consideration. z shear Symmetry axis For the cohesive surface, the constitutive behaviour is given in terms Substrate (elastic-plastic) ∆ (∆ ) n t of a traction versus separation law, where we have adopted the uni- versal binding law used by Xu and Needleman [1]. It is characterized mainly by the peak traction and the separation energy (Fig. 2). Results Figure 1. Geometry. Figure 2. Cohesive zone tractions. The energy for normal or shear separation is the area under the corresponding curve. Interfacial delamination: 0 σe/σy 0 1 σzz/σmax 1.40 1.00 1.20 shear delamination 0.75 0.8 normal delamination 1.00 0.50 50 0.80 20 0.25 0.60 0.6 F/Fmax 0.00 z (µm) z (µm) 0.40 -0.25 0.20 -0.50 0.4 100 40 0.2 (b) 0 150 (a) 60 0 0.5 1 1.5 2 0 50 100 150 0 20 40 60 h/t r (µm) r (µm) Figure 3. (a) Shear delamination . t = 5 µm, τ max = 1.2 GPa . Arrows show the shear direction, line Figure 4. Load versus displacement (F-h) curves for shows the location of the delaminated area. (b) Normal delamination. t = 2.5 µm, σ max = 1.5 GPa . Fig. 3. Coating cracking: 0 0 σrr/σmax σrr/σmax 1 e 2.00 2.00 1.56 1.56 d 5 0.8 1.11 5 1.11 0.67 0.67 0.22 0.22 0.6 F/Fmax z (µm) z (µm) 10 -0.22 10 -0.22 b c -0.67 -0.67 0.4 -1.11 -1.11 a 15 -1.56 15 -1.56 -2.00 -2.00 0.2 20 (a) 20 (b) 0 0 5 10 15 20 0 5 10 15 20 0 0.5 1 1.5 r (µm) r (µm) h/t Figure 5. Coating cracking. t = 2 µm, σ max = 11 GPa . (a) First crack at r 1 = 7.0 µm . (b) Second Figure 6. Load versus displacement curve for Fig. 5. crack at r 2 = 9.4 µm . Labelled points correspond to specific failure types. a and b on the curve correspond to mode I cracks at loca- tions r 1 and r 2 , respectively. At c the first crack grows Conclusions until the interface and at d it shears of f. Point e corre- sponds to some limited interfacial delamination in the 1. Shear delamination may occur in the loading stage. It is imprinted on the load vs displacement curve by a kink. vicinity of the coating cracks. 2. Normal delamination may occur during the unloading stage, where a circular part of the coating is lifted off from the substrate. It is imprinted on the load vs displacement curve by a hump. 3. Coating cracking may occur during the loading stage. The first circumferential crack occurs outside the con- tact area. The crack is imprinted on the F-h curve as a kink. 4. On further loading, subsequent cracking occurs with crack spacing of about 1.25 times the coating thickness. [1] X.-P. Xu, A. Needleman, Model. Simul. Mater. Sci. Eng. 1 (1993) 111.