Welding Practice
for the Sandvik Duplex Stainless Steels
SAF 2304, SAF 2205 and SAF 2507
Presented by
Frank Babish
Key Points
 Metallurgical Considerations
 Welding Processes
 Composition differences Base Metal and Filler Metal
 Good Mechanical and Corrosion Properties of Welds
 Importance of Heat Input and Interpass Temperature
 Role of Nitrogen
 Post Weld Cleaning
 Dissimiliar Joining
 Joint Design
Characteristics of
Duplex stainless steels
 Excellent resistance to stress corrosion cracking
 Very high mechanical strength
 Excellent resistance to pitting and crevice corrosion
 High resistance to general corrosion in a variety of
environments
 Low thermal expansion
 High resistance to erosion corrosion and corrosion
fatigue
 Good weldability
 Lower life cycle cost
Duplex microstructure
 The austenite islands
(light) are embedded in a
continuous ferrite (dark)
matrix.
 The duplex
microstructure typically
contains 45-65%
austenite and 35-55%
ferrite.
Austenite Ferrite
Yield Strength 0,2%
Austenitic vs Duplex Stainless Steel
0
400
500
600
200
300
100
316L
SAF
2304
904L
SAF
2205
6Mo+N
SAF
2507
Coefficient of expansion
(x10-6
)°C-1
Austenitic stainless steels approx. 17
Duplex stainless steels approx. 13
Carbon steel approx. 11,5
Thermal expansion, per °C (20-100°C)
0 5 10 15 20
Duplex
Carbon steel
AISI 316L
(x10-6
)
Solidification mechanism of
Duplex stainless steel
 As duplex stainless steels solidify the grain structure
transform from a fully ferritic material to a balanced
austenite and ferrite microstructure
Solidification mechanism of a
Duplex Stainless Steel
HAZ of weld in SAF 2507
Stress strain curves
Austenite, ferrite and duplex
0,0 0,2 0,4 0,6 0,8
0
200
400
600
800
1000
austenite
duplex (2205)
ferrite
Stress[MPa]
Strain
ferrite
duplex
austenite
Reasons for the high strength of
duplex stainless steels
 Content of ferrite
 Fine grained structure
 Nitrogen
Embrittling of Duplex Stainless Steels
Welding Processes
Conventional Processes
 GTAW
 GMAW
 SAW
 SMAW
 FCAW
Avoid
 Autogenous
 Low Energy Processes
 Or Perform PWHT
Filler Metals for the Welding of
Duplex Stainless Steels
Parent Welding Filler metalChemical composition, wt-%
metal process Sandvik C Si Mn P S Cr Ni Mo N Ferrite
Sandvik max. max. max. All weld
metal, %
SAF 2304 TIG, MIG, SAW 23.7.L 0,020 0,4 1,5 0,020 0,015 23 7 - 0,14 30-40
MMA 23.8.LR 0,030 <0,9 0,5 0,030 0,025 25 9 - 0,12 30-40
SAF 2304 TIG, MIG, SAW 2209 0.020 0,5 1,6 0,020 0.015 22,5 8 3 0,14 30-40
and MMA 2209-16,17 0,030 <1,0 0,8 0,030 0,025 22,5 9 3 0,12 30-40
SAF 2205 2209-15 0,04 <0,5 0,8 0,030 0,025 22 9 3 0,15 30-40
FCAW 2209LT 0.030 <1.0 1.5 0.030 0.025 22.5 9 3 0.15 30-40
SAF 2507 TIG, (MIG), SAW 25.10.4.L 0,020 0,3 0,4 0,020 0,020 25 10 4 0,25 30-40
MMA 25.10.4.LR 0,030 0,5 0,7 0,030 0,025 25 10 4 0,25 30-40
25.10.4.LB 0,040 0,4 0,9 0,030 0,025 25,5 9,5 4 0,25 30-40
Mechanical properties of the
Duplex Stainless Steels
Sandvik UNS Yield strength Tensile strength Elong. Hardness
0,2% offset 1,0% offset A5 Vickers
MPa ksi. MPa ksi. MPa ksi. %
min. min. min. min. min. min. min. approx.
SAF 2304 S32304 400 58 450 65 600-820 87-119 25 230
SAF 2205 S31803 450 65 500 73 680-880 99-128 25 260
SAF 2507 S32750 550 80 640 93 800-1000 116-145 25 290
Mechanical Properties of All Weld Metal
Filler metal Welding Rpo,2 Rp1,0 Rm A5 Z Impact strength, J
Sandvik process MPa MPa MPa % % RT -40°C
23.7.L TIG 525 595 708 34 58 171 156
23.7.L SAW1)
503 671 34 101 72
23.8.LR MMA 627 681 773 26 46 62 46
22.8.3.L TIG 610 760 28 207 160
22.8.3.L SAW1)
578 664 775 33 53 139 84
22.9.3.LR MMA 512 734 33 52 44
22.9.3.LT FCAW 620 - 816 30 44 56 43
25.10.4.L TIG 672 851 28 64 150 116
25.10.4.L SAW1)
687 757 878 27 47 91 64
25.10.4.LR MMA 645 850 28 46 33
1)
Using Sandvik 15W flux
Mechanical properties of welded joints.
Cross-weld tensile test
Parent metal Filler metal Welding Rp0.2 MPa
Sandvik Sandvik process min. typical
SAF 2304 23.7.L TIG 400 446
23.7.L SAW1)
400 452
23.8.LR MMA 400 462
SAF 2205 22.8.3.L TIG 450 553
22.8.3.L SAW1)
450 588
22.9.3.LR MMA 450 588
22.9.3.LT FCAW 450 585
SAF 2507 25.10.4.L TIG 550 645
25.10.4.L SAW1)
550 628
25.10.4.LR MMA 550 628
1)
Using Sandvik 15W flux
Charpy-V impact strength of welded joints
Parent metal Filler metal Welding Impact energy, J
Sandvik Sandvik process RT -40°C
SAF 2304 23.7.L TIG 213 74
23.7.L SAW1)
105 17
23.8.LR MMA 46 38
SAF 2205 22.8.3.L TIG 282 133
22.8.3.L SAW1)
54 42
22.9.3.LR MMA 52 43
22.9.3.LT FCAW55 44
SAF 2507 25.10.4.L TIG 110 78
25.10.4.L SAW1)
100 58
25.10.4.LR MMA 58 39
1)
Using Sandvik 15W flux
Typical CPT Values from G-48A Tests for Parent Metals and Welded Joints
Sandvik Filler Welding Shielding Root CPT °C
metal process gas gas
SAF 2304 ~15
All weld metal 23.7.L TIG Ar - <15
Joint 23.7.L TIG Ar Ar <15
Joint 23.7.L SAW1)
- - <15
Joint 23.8.LR MMA - - <15
SAF 2205 30
All weld metal 22.8.3.L TIG Ar - 20-23
Joint 22.8.3.L TIG Ar Ar 20-23
Joint 22.8.3.L TIG Ar - 2% N2 90 N2 + 10 H2 23-25
(or pure N2)
All weld metal 22.8.3.L SAW1)
- - 20-25
Joint 22.8.3.L SAW1)
- - 20-25
All weld metal 22.9.3.LR MMA - - 20-25
Joint 22.9.3.LR MMA - - 20-25
SAF 2507 80
Autogenous TIG welding 40
All weld metal 25.10.4.L TIG Ar - 40-45
Joint 25.10.4.L TIG Ar Ar 40-45
Joint 25.10.4.L TIG Ar 90 N2 + 10 H2 40-50
(or pure N2)
Joint 25.10.4.L TIG Ar + 2% N2 90 N2 + 10 H2 45-55
(or pure N2)
All weld metal 25.10.4.L SAW 1)
- - 40-50
Joint 25.10.4.L SAW 1)
- - 40-50
All weld metal 25.10.4.LR MMA - - 40-50
Joint 25.10.4.LR MMA - - 40-501)
Using Sandvik 15W flux
Quench annealing of Duplex Steel welds
Sandvik Holding temperature Quenching
°C media
SAF 2304 930 - 1050 Water
SAF 2205 1020 - 1100 Water
SAF 2507 1080 - 1120 Water
Chromium
nitrides Interm
etallics
High quenching temp
Rapid cooling
Low quenching temp.
Slow cooling
Intermetallic phase
Chromium
nitrides Interm
etallics
Recommended heat input
Steel Heat input Interpass temperature
SAF 2304 0,5 - 2,5 kJ/mm <250°C
SAF 2205 0,5 - 2,5 kJ/mm <250°C
SAF 2507 0,2 - 1,5 kJ/mm <150°C
Welding recommendations
Sandvik Heat input Interpass temperature
kJ/mm °C
SAF 2304 0,5 - 2,5 <250
SAF 2205 0,5 - 2,5 <250
SFA 2507 0,2 - 1,5 <150
The roll of Nitrogen
 Nitrogen is a very important alloying element in DSS
 Improves corrosion resistance
 Improves austenite reformation
 At TIG welding, the loss of nitrogen is compensated for by
using Ar + 1 - 2%N2 as a shielding gas
Ferritic area in SAF 2507 weld owing to the
loss of nitrogen in fusion line
Shielding gas Ar 99,99%
Nitrogen addition to the shielding gas
Ar 99,99% Ar + 5% N2
Ferrite content in TIG-welds, SAF 2507
Filler Shielding Root Ferrite content, v
metal gas gas + error with 95%
Sandvik confidence interv
25.10.4.L Ar Ar 55 + 4,5
25.10.4.L Ar 90% N2 + 10% H2 59 + 4,0
25.10.4.L Ar + 5% N2 90% N2 + 10% H2 33 + 4,0
Nitrogen Content in TIG welds of SAF 2507.
N=0,25% in the filler metal
Filler metal Shielding Root Weight-% N
Sandvik gas gas in deposit
25.10.4.L Ar 90% N2 + 10% H2 0,23
25.10.4.L Ar + 3% N2 90% N2 + 10% H2 0,27
25.10.4.L Ar + 6% N2 90% N2 + 10% H2 0,33
GMAW SHIELDING GASES
 General recommendations:
 Short arc welding gives very convex beads.
Ar+30 He+1 O2
 Spray arc welding
Ar+30 He+1 O2 (22Cr duplex)
Ar+2 CO2(Super duplex)
 Pulsed arc welding
Ar+30 He+1 O2 (22Cr duplex)
Ar(99,996%) for super duplex
Nitrogen Analysis from the Top of a TIG weld
% Nitrogen in position (o’clock) Analysis at
3 5 6 7 11 12
Welder No. 1 0,17 0,18 0,15 0,16 0,19 0,19 Top side
Welder No. 2 0,18 - 0,19 0,19 - Top side
0,20 - 0,21 0,20 - Root side
Welder No. 3 0,22 - 0,21 0,20 - Top side
0,21 - 0,21 0,20 - Root side
In all cases the filler metal had a nitrogen content of 0,25%
Stress relieving temperatures
325 + 25°C for 10 hours
Post Weld Cleaning
Pitting
potential
Pickling
bath or
pickling
paste
HNO3-HF
360 220 120 80 Wire
brush
Blasting
Dissimilar Joints
SAF Carbon steel AISI 200 AISI 904L,
and 300- Sanicro 28,
series 254 SMO, etc.
2304 22.8.3.L 22.8.3.L 22.8.3.L
22.9.3.LR 22.9.3.LR 22.9.3.LR
22.9.3.LT 22.9.3.LT 22.9.3.LT
2205 22.8.3.L 22.8.3.L 22.8.3.L
22.9.3.LR 22.9.3.LR 22.9.3.LR
22.9.3.LT 22.9.3.LT 22.9.3.LT
2507 25.10.4.L 25.10.4.L Sanicro 60
25.10.4.LR 25.10.4.LR Sanicro 60
Joint preparation
One sided butt welding
Joint preparation
Butt welding from both sides
Tube to tube sheet welding.
Joint preparation
>WT
>1.5 x WT
45°
>3 mm (0.12”) or >1.5 x WT
r >1.5 x WT
a b
c d
Hydrogen pick-up from covered electrodes
Sandvik 25.10.4.LR
MMA
H2, ml/100 g
0
5
10
15
Dried covering Covering exposed to
laboratory air
Moist covering
Hydrogen pick-up from SAW flux
0
5
10
15
Dried flux Moist flux
H2, ml/100 g
SAW
Hydrogen pick up from shielding gas
at TIG welding
0
5
10
15
Shielding gas
Ar + 5% H2
Shielding gas
Ar + 10% H2
TIG - no root gas
H2, ml/100 g
Hydrogen pick up from shielding gas
and root gas at TIG welding
0
5
10
15
TIG - with root gas
H2, ml/100 g
Shielding gas Ar
Root gas Ar
Shielding gas Ar
Root gas 90% N2 + 10% H2
Conclusions
Key Areas
 Good Weldability
 Uses Conventional Welding Processes
 Joint Design
 Role of Nitrogen
 Heat Input Important
 Interpass Temperature

Más contenido relacionado

La actualidad más candente

La actualidad más candente (20)

Welding of aluminum alloys
Welding of aluminum alloysWelding of aluminum alloys
Welding of aluminum alloys
 
Heat treatment part 2
Heat treatment part 2Heat treatment part 2
Heat treatment part 2
 
Guide Lines For Duplex Stainless Steel Welding
Guide Lines For Duplex Stainless Steel WeldingGuide Lines For Duplex Stainless Steel Welding
Guide Lines For Duplex Stainless Steel Welding
 
U5 p1 phase transformation
U5 p1 phase transformationU5 p1 phase transformation
U5 p1 phase transformation
 
Ttt diagram for eutectoid steel(bainite, spherodite, martensite)
Ttt diagram for eutectoid steel(bainite, spherodite, martensite)Ttt diagram for eutectoid steel(bainite, spherodite, martensite)
Ttt diagram for eutectoid steel(bainite, spherodite, martensite)
 
Welding of Titanium and Alloys
Welding of Titanium and AlloysWelding of Titanium and Alloys
Welding of Titanium and Alloys
 
Stainless steel
Stainless steelStainless steel
Stainless steel
 
Post-Weld-Heat-Treatment-ppt.ppt
Post-Weld-Heat-Treatment-ppt.pptPost-Weld-Heat-Treatment-ppt.ppt
Post-Weld-Heat-Treatment-ppt.ppt
 
Heat treatment of steel
Heat treatment of steelHeat treatment of steel
Heat treatment of steel
 
Heat affected zone
Heat affected zoneHeat affected zone
Heat affected zone
 
Hsla steels
Hsla steelsHsla steels
Hsla steels
 
Welding of non ferrous alloys
Welding of non ferrous alloysWelding of non ferrous alloys
Welding of non ferrous alloys
 
Maraging steel
Maraging steelMaraging steel
Maraging steel
 
Heat Treatment Lecture Notes
Heat Treatment Lecture NotesHeat Treatment Lecture Notes
Heat Treatment Lecture Notes
 
Heat Treatment Process
Heat Treatment ProcessHeat Treatment Process
Heat Treatment Process
 
Blast furnace presentation
Blast furnace presentation Blast furnace presentation
Blast furnace presentation
 
State of the Art in Vacuum Arc remelting and Electro Slag Remelting Process -...
State of the Art in Vacuum Arc remelting and Electro Slag Remelting Process -...State of the Art in Vacuum Arc remelting and Electro Slag Remelting Process -...
State of the Art in Vacuum Arc remelting and Electro Slag Remelting Process -...
 
STUDY OF MICROSTRUCTURE OF NON FERROUS METALS AND ALLOYS
STUDY OF MICROSTRUCTURE OF NON FERROUS METALS AND ALLOYSSTUDY OF MICROSTRUCTURE OF NON FERROUS METALS AND ALLOYS
STUDY OF MICROSTRUCTURE OF NON FERROUS METALS AND ALLOYS
 
Welding of ci
Welding of ciWelding of ci
Welding of ci
 
Welding of High Strength low Alloy (HSLA) Steels
Welding of High Strength low Alloy (HSLA)   SteelsWelding of High Strength low Alloy (HSLA)   Steels
Welding of High Strength low Alloy (HSLA) Steels
 

Similar a Welding duplex stainless steel

Williams Brochure Welding Products
Williams Brochure Welding ProductsWilliams Brochure Welding Products
Williams Brochure Welding Products
John Turley
 
Billets andbloomsfromcontinuouscasting
Billets andbloomsfromcontinuouscastingBillets andbloomsfromcontinuouscasting
Billets andbloomsfromcontinuouscasting
Kerem Demirbaş
 
Types%20of%20 Welding[1]
Types%20of%20 Welding[1]Types%20of%20 Welding[1]
Types%20of%20 Welding[1]
guestbd7851
 
Autogenous pulsed laser welding of aluminium alloy AA6082-T651
Autogenous pulsed laser welding of aluminium alloy AA6082-T651Autogenous pulsed laser welding of aluminium alloy AA6082-T651
Autogenous pulsed laser welding of aluminium alloy AA6082-T651
Rui Ravail Luz Rodrigues
 

Similar a Welding duplex stainless steel (20)

Williams Brochure Welding Products
Williams Brochure Welding ProductsWilliams Brochure Welding Products
Williams Brochure Welding Products
 
Materials11.pdf
Materials11.pdfMaterials11.pdf
Materials11.pdf
 
Alloy performance-guide
Alloy performance-guideAlloy performance-guide
Alloy performance-guide
 
Flux Cored - Arc Welding Wires
Flux Cored - Arc Welding WiresFlux Cored - Arc Welding Wires
Flux Cored - Arc Welding Wires
 
Types of welding
Types of weldingTypes of welding
Types of welding
 
Gas Metal Arc - Welding Wires (Solid Wires)
Gas Metal Arc - Welding Wires (Solid Wires)Gas Metal Arc - Welding Wires (Solid Wires)
Gas Metal Arc - Welding Wires (Solid Wires)
 
welding process
welding processwelding process
welding process
 
Cast iron
Cast ironCast iron
Cast iron
 
Billets andbloomsfromcontinuouscasting
Billets andbloomsfromcontinuouscastingBillets andbloomsfromcontinuouscasting
Billets andbloomsfromcontinuouscasting
 
Standard cr ni-mo-stainless_steels_datasheet
Standard cr ni-mo-stainless_steels_datasheetStandard cr ni-mo-stainless_steels_datasheet
Standard cr ni-mo-stainless_steels_datasheet
 
Fusion Welding Parameters
Fusion Welding ParametersFusion Welding Parameters
Fusion Welding Parameters
 
Types%20of%20 Welding[1]
Types%20of%20 Welding[1]Types%20of%20 Welding[1]
Types%20of%20 Welding[1]
 
MIG/TIG - Welding Consumables
MIG/TIG - Welding ConsumablesMIG/TIG - Welding Consumables
MIG/TIG - Welding Consumables
 
Jr2517091717
Jr2517091717Jr2517091717
Jr2517091717
 
Jr2517091717
Jr2517091717Jr2517091717
Jr2517091717
 
Welding of aluminium castings - October 2011
Welding of aluminium castings - October 2011Welding of aluminium castings - October 2011
Welding of aluminium castings - October 2011
 
Astm a409 a409-m-01(r05)
Astm a409 a409-m-01(r05)Astm a409 a409-m-01(r05)
Astm a409 a409-m-01(r05)
 
Korean stainless wire &amp; cable b2 k
Korean stainless wire &amp; cable  b2 kKorean stainless wire &amp; cable  b2 k
Korean stainless wire &amp; cable b2 k
 
Asme section ii c new
Asme section ii c newAsme section ii c new
Asme section ii c new
 
Autogenous pulsed laser welding of aluminium alloy AA6082-T651
Autogenous pulsed laser welding of aluminium alloy AA6082-T651Autogenous pulsed laser welding of aluminium alloy AA6082-T651
Autogenous pulsed laser welding of aluminium alloy AA6082-T651
 

Último

AKTU Computer Networks notes --- Unit 3.pdf
AKTU Computer Networks notes ---  Unit 3.pdfAKTU Computer Networks notes ---  Unit 3.pdf
AKTU Computer Networks notes --- Unit 3.pdf
ankushspencer015
 
notes on Evolution Of Analytic Scalability.ppt
notes on Evolution Of Analytic Scalability.pptnotes on Evolution Of Analytic Scalability.ppt
notes on Evolution Of Analytic Scalability.ppt
MsecMca
 
Call Girls In Bangalore ☎ 7737669865 🥵 Book Your One night Stand
Call Girls In Bangalore ☎ 7737669865 🥵 Book Your One night StandCall Girls In Bangalore ☎ 7737669865 🥵 Book Your One night Stand
Call Girls In Bangalore ☎ 7737669865 🥵 Book Your One night Stand
amitlee9823
 
Call for Papers - African Journal of Biological Sciences, E-ISSN: 2663-2187, ...
Call for Papers - African Journal of Biological Sciences, E-ISSN: 2663-2187, ...Call for Papers - African Journal of Biological Sciences, E-ISSN: 2663-2187, ...
Call for Papers - African Journal of Biological Sciences, E-ISSN: 2663-2187, ...
Christo Ananth
 

Último (20)

Thermal Engineering -unit - III & IV.ppt
Thermal Engineering -unit - III & IV.pptThermal Engineering -unit - III & IV.ppt
Thermal Engineering -unit - III & IV.ppt
 
Thermal Engineering Unit - I & II . ppt
Thermal Engineering  Unit - I & II . pptThermal Engineering  Unit - I & II . ppt
Thermal Engineering Unit - I & II . ppt
 
AKTU Computer Networks notes --- Unit 3.pdf
AKTU Computer Networks notes ---  Unit 3.pdfAKTU Computer Networks notes ---  Unit 3.pdf
AKTU Computer Networks notes --- Unit 3.pdf
 
(INDIRA) Call Girl Bhosari Call Now 8617697112 Bhosari Escorts 24x7
(INDIRA) Call Girl Bhosari Call Now 8617697112 Bhosari Escorts 24x7(INDIRA) Call Girl Bhosari Call Now 8617697112 Bhosari Escorts 24x7
(INDIRA) Call Girl Bhosari Call Now 8617697112 Bhosari Escorts 24x7
 
Vivazz, Mieres Social Housing Design Spain
Vivazz, Mieres Social Housing Design SpainVivazz, Mieres Social Housing Design Spain
Vivazz, Mieres Social Housing Design Spain
 
Double rodded leveling 1 pdf activity 01
Double rodded leveling 1 pdf activity 01Double rodded leveling 1 pdf activity 01
Double rodded leveling 1 pdf activity 01
 
notes on Evolution Of Analytic Scalability.ppt
notes on Evolution Of Analytic Scalability.pptnotes on Evolution Of Analytic Scalability.ppt
notes on Evolution Of Analytic Scalability.ppt
 
VIP Model Call Girls Kothrud ( Pune ) Call ON 8005736733 Starting From 5K to ...
VIP Model Call Girls Kothrud ( Pune ) Call ON 8005736733 Starting From 5K to ...VIP Model Call Girls Kothrud ( Pune ) Call ON 8005736733 Starting From 5K to ...
VIP Model Call Girls Kothrud ( Pune ) Call ON 8005736733 Starting From 5K to ...
 
(INDIRA) Call Girl Aurangabad Call Now 8617697112 Aurangabad Escorts 24x7
(INDIRA) Call Girl Aurangabad Call Now 8617697112 Aurangabad Escorts 24x7(INDIRA) Call Girl Aurangabad Call Now 8617697112 Aurangabad Escorts 24x7
(INDIRA) Call Girl Aurangabad Call Now 8617697112 Aurangabad Escorts 24x7
 
Call Girls Wakad Call Me 7737669865 Budget Friendly No Advance Booking
Call Girls Wakad Call Me 7737669865 Budget Friendly No Advance BookingCall Girls Wakad Call Me 7737669865 Budget Friendly No Advance Booking
Call Girls Wakad Call Me 7737669865 Budget Friendly No Advance Booking
 
Call Girls In Bangalore ☎ 7737669865 🥵 Book Your One night Stand
Call Girls In Bangalore ☎ 7737669865 🥵 Book Your One night StandCall Girls In Bangalore ☎ 7737669865 🥵 Book Your One night Stand
Call Girls In Bangalore ☎ 7737669865 🥵 Book Your One night Stand
 
Double Revolving field theory-how the rotor develops torque
Double Revolving field theory-how the rotor develops torqueDouble Revolving field theory-how the rotor develops torque
Double Revolving field theory-how the rotor develops torque
 
Call for Papers - African Journal of Biological Sciences, E-ISSN: 2663-2187, ...
Call for Papers - African Journal of Biological Sciences, E-ISSN: 2663-2187, ...Call for Papers - African Journal of Biological Sciences, E-ISSN: 2663-2187, ...
Call for Papers - African Journal of Biological Sciences, E-ISSN: 2663-2187, ...
 
Top Rated Pune Call Girls Budhwar Peth ⟟ 6297143586 ⟟ Call Me For Genuine Se...
Top Rated  Pune Call Girls Budhwar Peth ⟟ 6297143586 ⟟ Call Me For Genuine Se...Top Rated  Pune Call Girls Budhwar Peth ⟟ 6297143586 ⟟ Call Me For Genuine Se...
Top Rated Pune Call Girls Budhwar Peth ⟟ 6297143586 ⟟ Call Me For Genuine Se...
 
Intze Overhead Water Tank Design by Working Stress - IS Method.pdf
Intze Overhead Water Tank  Design by Working Stress - IS Method.pdfIntze Overhead Water Tank  Design by Working Stress - IS Method.pdf
Intze Overhead Water Tank Design by Working Stress - IS Method.pdf
 
Unleashing the Power of the SORA AI lastest leap
Unleashing the Power of the SORA AI lastest leapUnleashing the Power of the SORA AI lastest leap
Unleashing the Power of the SORA AI lastest leap
 
The Most Attractive Pune Call Girls Manchar 8250192130 Will You Miss This Cha...
The Most Attractive Pune Call Girls Manchar 8250192130 Will You Miss This Cha...The Most Attractive Pune Call Girls Manchar 8250192130 Will You Miss This Cha...
The Most Attractive Pune Call Girls Manchar 8250192130 Will You Miss This Cha...
 
PVC VS. FIBERGLASS (FRP) GRAVITY SEWER - UNI BELL
PVC VS. FIBERGLASS (FRP) GRAVITY SEWER - UNI BELLPVC VS. FIBERGLASS (FRP) GRAVITY SEWER - UNI BELL
PVC VS. FIBERGLASS (FRP) GRAVITY SEWER - UNI BELL
 
KubeKraft presentation @CloudNativeHooghly
KubeKraft presentation @CloudNativeHooghlyKubeKraft presentation @CloudNativeHooghly
KubeKraft presentation @CloudNativeHooghly
 
Booking open Available Pune Call Girls Koregaon Park 6297143586 Call Hot Ind...
Booking open Available Pune Call Girls Koregaon Park  6297143586 Call Hot Ind...Booking open Available Pune Call Girls Koregaon Park  6297143586 Call Hot Ind...
Booking open Available Pune Call Girls Koregaon Park 6297143586 Call Hot Ind...
 

Welding duplex stainless steel

  • 1. This Presentation is provided to you by: WPSAmerica.com Industry Standard Welding Procedures Software for AWS and ASME Codes
  • 2. Welding Practice for the Sandvik Duplex Stainless Steels SAF 2304, SAF 2205 and SAF 2507 Presented by Frank Babish
  • 3. Key Points  Metallurgical Considerations  Welding Processes  Composition differences Base Metal and Filler Metal  Good Mechanical and Corrosion Properties of Welds  Importance of Heat Input and Interpass Temperature  Role of Nitrogen  Post Weld Cleaning  Dissimiliar Joining  Joint Design
  • 4. Characteristics of Duplex stainless steels  Excellent resistance to stress corrosion cracking  Very high mechanical strength  Excellent resistance to pitting and crevice corrosion  High resistance to general corrosion in a variety of environments  Low thermal expansion  High resistance to erosion corrosion and corrosion fatigue  Good weldability  Lower life cycle cost
  • 5. Duplex microstructure  The austenite islands (light) are embedded in a continuous ferrite (dark) matrix.  The duplex microstructure typically contains 45-65% austenite and 35-55% ferrite. Austenite Ferrite
  • 6. Yield Strength 0,2% Austenitic vs Duplex Stainless Steel 0 400 500 600 200 300 100 316L SAF 2304 904L SAF 2205 6Mo+N SAF 2507
  • 7. Coefficient of expansion (x10-6 )°C-1 Austenitic stainless steels approx. 17 Duplex stainless steels approx. 13 Carbon steel approx. 11,5
  • 8. Thermal expansion, per °C (20-100°C) 0 5 10 15 20 Duplex Carbon steel AISI 316L (x10-6 )
  • 9. Solidification mechanism of Duplex stainless steel  As duplex stainless steels solidify the grain structure transform from a fully ferritic material to a balanced austenite and ferrite microstructure
  • 10. Solidification mechanism of a Duplex Stainless Steel
  • 11. HAZ of weld in SAF 2507
  • 12. Stress strain curves Austenite, ferrite and duplex 0,0 0,2 0,4 0,6 0,8 0 200 400 600 800 1000 austenite duplex (2205) ferrite Stress[MPa] Strain ferrite duplex austenite
  • 13. Reasons for the high strength of duplex stainless steels  Content of ferrite  Fine grained structure  Nitrogen
  • 14. Embrittling of Duplex Stainless Steels
  • 15. Welding Processes Conventional Processes  GTAW  GMAW  SAW  SMAW  FCAW Avoid  Autogenous  Low Energy Processes  Or Perform PWHT
  • 16. Filler Metals for the Welding of Duplex Stainless Steels Parent Welding Filler metalChemical composition, wt-% metal process Sandvik C Si Mn P S Cr Ni Mo N Ferrite Sandvik max. max. max. All weld metal, % SAF 2304 TIG, MIG, SAW 23.7.L 0,020 0,4 1,5 0,020 0,015 23 7 - 0,14 30-40 MMA 23.8.LR 0,030 <0,9 0,5 0,030 0,025 25 9 - 0,12 30-40 SAF 2304 TIG, MIG, SAW 2209 0.020 0,5 1,6 0,020 0.015 22,5 8 3 0,14 30-40 and MMA 2209-16,17 0,030 <1,0 0,8 0,030 0,025 22,5 9 3 0,12 30-40 SAF 2205 2209-15 0,04 <0,5 0,8 0,030 0,025 22 9 3 0,15 30-40 FCAW 2209LT 0.030 <1.0 1.5 0.030 0.025 22.5 9 3 0.15 30-40 SAF 2507 TIG, (MIG), SAW 25.10.4.L 0,020 0,3 0,4 0,020 0,020 25 10 4 0,25 30-40 MMA 25.10.4.LR 0,030 0,5 0,7 0,030 0,025 25 10 4 0,25 30-40 25.10.4.LB 0,040 0,4 0,9 0,030 0,025 25,5 9,5 4 0,25 30-40
  • 17. Mechanical properties of the Duplex Stainless Steels Sandvik UNS Yield strength Tensile strength Elong. Hardness 0,2% offset 1,0% offset A5 Vickers MPa ksi. MPa ksi. MPa ksi. % min. min. min. min. min. min. min. approx. SAF 2304 S32304 400 58 450 65 600-820 87-119 25 230 SAF 2205 S31803 450 65 500 73 680-880 99-128 25 260 SAF 2507 S32750 550 80 640 93 800-1000 116-145 25 290
  • 18. Mechanical Properties of All Weld Metal Filler metal Welding Rpo,2 Rp1,0 Rm A5 Z Impact strength, J Sandvik process MPa MPa MPa % % RT -40°C 23.7.L TIG 525 595 708 34 58 171 156 23.7.L SAW1) 503 671 34 101 72 23.8.LR MMA 627 681 773 26 46 62 46 22.8.3.L TIG 610 760 28 207 160 22.8.3.L SAW1) 578 664 775 33 53 139 84 22.9.3.LR MMA 512 734 33 52 44 22.9.3.LT FCAW 620 - 816 30 44 56 43 25.10.4.L TIG 672 851 28 64 150 116 25.10.4.L SAW1) 687 757 878 27 47 91 64 25.10.4.LR MMA 645 850 28 46 33 1) Using Sandvik 15W flux
  • 19. Mechanical properties of welded joints. Cross-weld tensile test Parent metal Filler metal Welding Rp0.2 MPa Sandvik Sandvik process min. typical SAF 2304 23.7.L TIG 400 446 23.7.L SAW1) 400 452 23.8.LR MMA 400 462 SAF 2205 22.8.3.L TIG 450 553 22.8.3.L SAW1) 450 588 22.9.3.LR MMA 450 588 22.9.3.LT FCAW 450 585 SAF 2507 25.10.4.L TIG 550 645 25.10.4.L SAW1) 550 628 25.10.4.LR MMA 550 628 1) Using Sandvik 15W flux
  • 20. Charpy-V impact strength of welded joints Parent metal Filler metal Welding Impact energy, J Sandvik Sandvik process RT -40°C SAF 2304 23.7.L TIG 213 74 23.7.L SAW1) 105 17 23.8.LR MMA 46 38 SAF 2205 22.8.3.L TIG 282 133 22.8.3.L SAW1) 54 42 22.9.3.LR MMA 52 43 22.9.3.LT FCAW55 44 SAF 2507 25.10.4.L TIG 110 78 25.10.4.L SAW1) 100 58 25.10.4.LR MMA 58 39 1) Using Sandvik 15W flux
  • 21. Typical CPT Values from G-48A Tests for Parent Metals and Welded Joints Sandvik Filler Welding Shielding Root CPT °C metal process gas gas SAF 2304 ~15 All weld metal 23.7.L TIG Ar - <15 Joint 23.7.L TIG Ar Ar <15 Joint 23.7.L SAW1) - - <15 Joint 23.8.LR MMA - - <15 SAF 2205 30 All weld metal 22.8.3.L TIG Ar - 20-23 Joint 22.8.3.L TIG Ar Ar 20-23 Joint 22.8.3.L TIG Ar - 2% N2 90 N2 + 10 H2 23-25 (or pure N2) All weld metal 22.8.3.L SAW1) - - 20-25 Joint 22.8.3.L SAW1) - - 20-25 All weld metal 22.9.3.LR MMA - - 20-25 Joint 22.9.3.LR MMA - - 20-25 SAF 2507 80 Autogenous TIG welding 40 All weld metal 25.10.4.L TIG Ar - 40-45 Joint 25.10.4.L TIG Ar Ar 40-45 Joint 25.10.4.L TIG Ar 90 N2 + 10 H2 40-50 (or pure N2) Joint 25.10.4.L TIG Ar + 2% N2 90 N2 + 10 H2 45-55 (or pure N2) All weld metal 25.10.4.L SAW 1) - - 40-50 Joint 25.10.4.L SAW 1) - - 40-50 All weld metal 25.10.4.LR MMA - - 40-50 Joint 25.10.4.LR MMA - - 40-501) Using Sandvik 15W flux
  • 22. Quench annealing of Duplex Steel welds Sandvik Holding temperature Quenching °C media SAF 2304 930 - 1050 Water SAF 2205 1020 - 1100 Water SAF 2507 1080 - 1120 Water
  • 23. Chromium nitrides Interm etallics High quenching temp Rapid cooling Low quenching temp. Slow cooling
  • 25. Chromium nitrides Interm etallics Recommended heat input Steel Heat input Interpass temperature SAF 2304 0,5 - 2,5 kJ/mm <250°C SAF 2205 0,5 - 2,5 kJ/mm <250°C SAF 2507 0,2 - 1,5 kJ/mm <150°C
  • 26. Welding recommendations Sandvik Heat input Interpass temperature kJ/mm °C SAF 2304 0,5 - 2,5 <250 SAF 2205 0,5 - 2,5 <250 SFA 2507 0,2 - 1,5 <150
  • 27. The roll of Nitrogen  Nitrogen is a very important alloying element in DSS  Improves corrosion resistance  Improves austenite reformation  At TIG welding, the loss of nitrogen is compensated for by using Ar + 1 - 2%N2 as a shielding gas
  • 28. Ferritic area in SAF 2507 weld owing to the loss of nitrogen in fusion line Shielding gas Ar 99,99%
  • 29. Nitrogen addition to the shielding gas Ar 99,99% Ar + 5% N2
  • 30. Ferrite content in TIG-welds, SAF 2507 Filler Shielding Root Ferrite content, v metal gas gas + error with 95% Sandvik confidence interv 25.10.4.L Ar Ar 55 + 4,5 25.10.4.L Ar 90% N2 + 10% H2 59 + 4,0 25.10.4.L Ar + 5% N2 90% N2 + 10% H2 33 + 4,0
  • 31. Nitrogen Content in TIG welds of SAF 2507. N=0,25% in the filler metal Filler metal Shielding Root Weight-% N Sandvik gas gas in deposit 25.10.4.L Ar 90% N2 + 10% H2 0,23 25.10.4.L Ar + 3% N2 90% N2 + 10% H2 0,27 25.10.4.L Ar + 6% N2 90% N2 + 10% H2 0,33
  • 32. GMAW SHIELDING GASES  General recommendations:  Short arc welding gives very convex beads. Ar+30 He+1 O2  Spray arc welding Ar+30 He+1 O2 (22Cr duplex) Ar+2 CO2(Super duplex)  Pulsed arc welding Ar+30 He+1 O2 (22Cr duplex) Ar(99,996%) for super duplex
  • 33. Nitrogen Analysis from the Top of a TIG weld % Nitrogen in position (o’clock) Analysis at 3 5 6 7 11 12 Welder No. 1 0,17 0,18 0,15 0,16 0,19 0,19 Top side Welder No. 2 0,18 - 0,19 0,19 - Top side 0,20 - 0,21 0,20 - Root side Welder No. 3 0,22 - 0,21 0,20 - Top side 0,21 - 0,21 0,20 - Root side In all cases the filler metal had a nitrogen content of 0,25%
  • 34. Stress relieving temperatures 325 + 25°C for 10 hours
  • 35. Post Weld Cleaning Pitting potential Pickling bath or pickling paste HNO3-HF 360 220 120 80 Wire brush Blasting
  • 36. Dissimilar Joints SAF Carbon steel AISI 200 AISI 904L, and 300- Sanicro 28, series 254 SMO, etc. 2304 22.8.3.L 22.8.3.L 22.8.3.L 22.9.3.LR 22.9.3.LR 22.9.3.LR 22.9.3.LT 22.9.3.LT 22.9.3.LT 2205 22.8.3.L 22.8.3.L 22.8.3.L 22.9.3.LR 22.9.3.LR 22.9.3.LR 22.9.3.LT 22.9.3.LT 22.9.3.LT 2507 25.10.4.L 25.10.4.L Sanicro 60 25.10.4.LR 25.10.4.LR Sanicro 60
  • 39. Tube to tube sheet welding. Joint preparation >WT >1.5 x WT 45° >3 mm (0.12”) or >1.5 x WT r >1.5 x WT a b c d
  • 40. Hydrogen pick-up from covered electrodes Sandvik 25.10.4.LR MMA H2, ml/100 g 0 5 10 15 Dried covering Covering exposed to laboratory air Moist covering
  • 41. Hydrogen pick-up from SAW flux 0 5 10 15 Dried flux Moist flux H2, ml/100 g SAW
  • 42. Hydrogen pick up from shielding gas at TIG welding 0 5 10 15 Shielding gas Ar + 5% H2 Shielding gas Ar + 10% H2 TIG - no root gas H2, ml/100 g
  • 43. Hydrogen pick up from shielding gas and root gas at TIG welding 0 5 10 15 TIG - with root gas H2, ml/100 g Shielding gas Ar Root gas Ar Shielding gas Ar Root gas 90% N2 + 10% H2
  • 44. Conclusions Key Areas  Good Weldability  Uses Conventional Welding Processes  Joint Design  Role of Nitrogen  Heat Input Important  Interpass Temperature